Mefuta e Meraro ea Mekhoa ea ho Qhibilihisa le Ho Tšela Bakeng sa Ductile Iron
Lehlabathe la lehoakhoa la Furan hangata le sebelisoa e le thepa ea ho bopa bakeng sa litšepe tse kholo tsa ductile tse hlahisoang Chaena. E hlahisoa ka sekhechana se le seng, ka boima bo boima ba ho tšela le sebopeho se rarahaneng. E na le litlhoko tse phahameng boleng le ts'ebetso ea li-castings. Liphoso tse ling tsa ho lahla, haholo liphoso tsa shrinkage, hangata li hlaha ts'ebetsong ea ho qhibilihisa. E tla etsa hore ho betloa ho hlakoloe mme ho bake tahlehelo e kholo ea moruo, haholo-holo thepa ea QT400-18AR, e nang le matla a phahameng, bophahamo bo phahameng, le litlhoko tsa boleng ba boleng.
Ha re ntse re netefatsa litšobotsi tsa mochini oa likarolo tse tenya le tse kholo joalo, ha ho bonolo ho qoba liphoso tsa graphite tse phaphametseng le tse nyenyefatsang. Ka moralo oa liteko tsa sampole, lisebelisoa tsa tlhaiso-leseling tsa Elkem li ile tsa sebelisoa ho ithuta litlamorao tsa sebopeho sa lik'hemik'hale le ho tšolla mocheso ho graphite e phaphametseng, shrinkage le liphoso tse ling tsa sampole e tiileng e nang le botenya ba lebota la 180mm. E sebelisoa ho tlhahiso ea likarolo tse nang le marako a tšepe a ductile ho fumana boleng bo holimo.
Lisebelisoa le lisebelisuoa li lokiselitsoe tšebeliso ea tšepe ea kolobe e hloekileng haholo, masala a hloekileng a manganese, sesebelisoa se phahameng sa magnesium spheroidizing, 75 # FeSi inoculant; Elkem low-magnesium spheroidizing agent, inoculant; Lithane tsa 1.5 tsa sebōpi se qhibilihisang maqhubu a mahareng, 500kg spheroidizing bag, 500kg tundish. Elkem EPIC thermal analyzer, k'harase ea sebabole le sebabole, sebali sa motlakase. Boholo ba mohlala o tiileng oa lehong ke 600mm × 400mm × 180mm, mme ts'ebetso e hlahisoa ka liteko. Lerako la botenya ba 180mm le sebelisetsoa ho koahela lihlahisoa tse thata le tse kholo tsa spheroidal graphite cast iron tse hlahisoang ke k'hamphani. E emetse haholo. E na le sistimi ea riser le sprue mme e tšela tlase e tšela ka boima bo tšollang ba 500kg.
Morero oa ho qhibilihisa le oa ho tšollela o etselitsoe ho sebelisa sebōpi sa maqhubu a 1.5t se qhibilihisang maqhubu ho qhibilihisa tšepe ea 1.5t e qhibilihisitsoeng, 500kg nako le nako ha e qhekella, le ho tšela lebokose le le leng la likotoana tsa liteko. Kakaretso ea mabokose a 1 a likotoana tsa liteko a ile a tšeloa seboping se le seng. Merero e fapaneng ea ho qhibilihisa le ho tšolla e entsoe ka tsela e latelang:
Sekhahla sa pele sa tefiso ea sekema:
85% ea tšepe ea kolobe, 15% sesebelisoa sa tšepe ea manganese e tlase; taolo ea lik'hemik'hale: amohela moralo oa kalafo ea spheroidizing inoculation: pele, tšepe ea 500kg e isoa ho tundish, mme 1.3-1.5% high-magnesium spheroidizing agent, 0.3-0.4% inoculant le inoculant li kentsoe ka mokotleng oa spheroidizing 0.8% e koahelang moemeli, invert mokotla bakeng sa spheroidization. Kamora hore ts'ebetso ea spheroidization e phetheloe, bokaholimo ba mokotla bo tšeloa ka phallo ea ente ebe e soasoa ka botlalo, ebe sampole e ea hlahlojoa le ho hlahlojoa ka seletsa sa EPIC. 1.2% Elkem spheroidizing agent, 0.8-1.0% e koahelang moemeli, le 0.4% khalase ea khalase e kentsoe ka mokotleng oa spheroidizing, 'me tšepe e kenella ka kotloloho ka mokotleng oa spheroidizing,' me 0.5% ea Elkem inoculant e kenngoa ka nako e le 'ngoe. Kamora hore spheroidization e phetheloe, ente e latelang ea Elkem e fafalitsoeng ka holim'a metsi e tla hlahlojoa le ho hlahlojoa ho sebelisoa seletsa sa EPIC.
1.2% Elkem spheroidizing agent, 0.8-1.0% e koahelang moemeli, le 0.4% khalase ea khalase e kentsoe ka mokotleng oa spheroidizing, 'me tšepe e kenella ka kotloloho ka mokotleng oa spheroidizing,' me 0.5% ea Elkem inoculant e kenngoa ka nako e le 'ngoe. Kamora hore spheroidization e phetheloe, ente e latelang ea Elkem e fafalitsoeng ka holim'a metsi e tla hlahlojoa le ho hlahlojoa ho sebelisoa seletsa sa EPIC.
Sekhahla sa bobeli sa tefiso ea sekhahla: 65% ea tšepe ea kolobe, 35% sephephechaneng sa manganese se tlaase; taolo ea lik'hemik'hale
C | Si | Mn | P | S | Cu | |
Sebopi sa pele | 3.7-3.9 | 0.6-0.75 | 0.1-0.25 |
Ho amohela moralo oa kalafo ea spheroidizing inoculation: lebisa 500kg ea tšepe ho tundish, e kentsoeng 1.2% Elkem nodulizer, 0.8-1.0% e koahelang moemeli le 0.4% ea khalase ea mokotla ka mokotleng oa spheroidizing, le tšepe e lebisang ho mokotla oa nodularizing. Kenya inoculant ea 0.5% ea Elkem. Kamora hore ts'ebetso ea spheroidization e phetheloe, beha ente e kenang ea Elkem ka har'a mokotla, o e pshatle ka botlalo, 'me u sebelise seletsa sa EPIC bakeng sa ho hlahloba le ho etsa liteko.
500kg ea tšepe e ka tlhatsoa ka kotloloho ho tundish, mme 0.95% Elkem low-magnesium spheroidizing agent, 0.65% Elkem e koahelang moemeli, 0.2% sesebelisoa sa tšepe le 0.1% slag remover li kentsoe ka mokotleng oa spheroidizing, 'me tšepe e ka ts'oaroa ka kotloloho ho spheroidizing sephutheloana. Kamora hore spheroidization e phetheloe, ente e latelang ea Elkem e fafatsoa ka holim'a metsi, e sentsoe ka botlalo, mme sampole e hlahlojoa le ho hlahlojoa ka seletsa sa EPIC. Tlanya ka kotloloho tšepe ea 500kg ho tundish, 'me mokotla oa spheroidizing o kentsoe 1.2% Elkem nodulizer, 0.3% e koahelang moemeli, 0.2% Elkem inoculant, 0.5% sephephechaneng sa tšepe le 0.1% slag remover, ka ho toba tsoa Iron ka mokotleng oa spheroidizing, le ka nako e ts'oanang beha 0.35% ea Elkem inoculant.
Kamora hore spheroidization e phetheloe, ente e latelang ea Elkem e fafatsoa ka holim'a metsi, e sentsoe ka botlalo, mme sampole e hlahlojoa le ho hlahlojoa ka seletsa sa EPIC. Morero oa boraro ke karolelano ea tefiso: 65% ea tšepe ea kolobe, 35% ea litšila; taolo ea sebopeho sa lik'hemik'hale:
C | Si | Mn | P | S | Cu | |
Sebopi sa pele | 3.8-4.0 | 1.1-1.4 | 0.1-0.25 |
Morero oa kalafo ea spheroidization inoculation oa amoheloa: tšepe ea 500kg e tobetsoe ka kotloloho ho tundish, 1.2% Elkem low-magnesium spheroidizing agent, 0.8% e koahelang moemeli le 0.1% slag remover e kentsoe ka mokotleng oa spheroidizing, 'me tšepe e tobisoa ka kotloloho ho mokotla oa spheroidizing. Ka nako e ts'oanang, 0.55% ea Elkem inoculant e kentsoe ho eona. Kamora hore ts'ebetso ea spheroidization e phethoe, phallo ea phallo ea Elkem e ile ea beoa bokaholimo ba mokotla o neng o sentsoe ka botlalo, mme mehlala e ile ea hlahlojoa le ho lekoa ka seletsa sa EPIC. Tlanya ka kotloloho tšepe ea 500kg ho tundish, e kentsoeng 1.2% Elkem low-magnesium spheroidizing agent, 0.8% Elkem e koahelang moemeli, le 0.1% slag remover ka mokotleng oa spheroidizing, tlanya tšepe ka kotloloho ho mokotla oa spheroidizing, 'me ka nako e ts'oanang tsetela 0.55 % Ente ea Elkem. Kamora hore spheroidization e phetheloe, ente e latelang ea Elkem e fafalitsoeng ka holim'a metsi e soahlamane ka botlalo, mme sampole e hlahlojoa le ho hlahlojoa ka seletsa sa EPIC. Tlanya ka kotloloho tšepe ea 500kg ho tundish, le pre-embed 1.2% Elkem low-magnesium spheroidizing agent, 0.3% e koahelang moemeli, 0.2% Elkem inoculant le 0.1% slag remover ka mokotleng oa spheroidizing, tlanya ka ho otloloha tšepe ho spheroidizing Package, ha o ntse o beha ka 0.35% ente ea Elkem. Kamora hore spheroidization e phetheloe, ente ea Elkem e fafalitsoeng ka holim'a metsi e soahlamana ka botlalo, mme sampole e hlahlojoa le ho hlahlojoa ka seletsa sa EPIC. Mekhoa ea tlhahlobo ea tlhahlobo le mekhoa ea ho e lekola Likateng tsa khabone le sebabole tsa tšepe e entsoeng ka ho qhibilihisoa li fumanoa ke sesebelisoa sa khabone le sebabole, 'me litaba tsa lits'epe tse kopantsoeng tse kang P, Mn le Cu li fumanoa ke mohlahlobi oa lipalo; Mothinya o pholileng oa mefuta e fapaneng ea lik'hemik'hale ka pele ho sebōpi o fumanoa ke thepa ea Elkem EPIC. Mohlala, LET (mocheso oa mokelikeli oa phetoho ea mokelikeli), CE (e lekanang le khabone), G1, G2, le G3 li na le mekhahlelo e fapaneng ea linako. Liphetho tsa liteko le puisano Liphetho le puisano ea morero oa pele:
C | Si | Mn | P | S | Cu | |
1-1 | 3.40 | 2.51 | 0.20 | 0.007 | 0.14 | |
1-2 | 3.45 | 1.90 | 0.18 | 0.010 | 0.14 | |
1-3 | 3.30 | 2.61 | 0.18 | 0.013 | 0.14 |
Ho latela mekhoa e fapaneng ea ts'ebetso, litšoantšo tse fumanoeng tsa EPIC ke tse latelang:
Mothinya 1: Mothinya oa sebopi sa pele se qhibilihisitsoeng sa molora oa molora oa molora
Mothapo oa 2: Sephetho sa sephetho sa sebōpi sa pele sa A
Mothapo oa 3: sekhahla sa sephetho sa sebōpi sa pele sa B sa 4: sephetho sa sekema sa pele sa sebōpi C.
- Ho tloha ho li-curve 1 le 2, rea bona hore boleng ba LET ba sekema sa pele sa sebōpi A boa eketseha kamora ts'ebetso ea spheroidization, e bonts'a karolo ea eona ea mokelikeli Mocheso o lekanang oa eketseha, empa karohano ea G1 e ntse e le kholo ho 34%, 'me LET -ST Nako ea pula ea graphite ke metsotsoana e 115. E kopantsoe le lik'hemik'hale tsa eona, hoa tsebahala hore khabone e lekanang le eona ke eona e phahameng ka ho fetisisa har'a litharollo tse tharo seboping sa pele.
- Ho tloha ho li-curve 1 le 3, rea bona hore boleng ba LET boa nyoloha ho tloha ho 1132 ho isa 1146 ° C, karohano ea G1 ke 36%, 'me nako ea pula ea LET-ST graphite ke metsotsoana e 129. E kopantsoe le lik'hemik'hale tsa eona, rea tseba hore k'habone e lekanang le eona ke ea pele Ho tse tlase ka ho fetisisa likhethong tse tharo seboping se le seng.
- Ho tloha ho li-curve 1 le 4, rea bona hore ha boleng ba LET bo eketseha ho tloha ho 1132 ho isa 1140, karohano ea G1 ke 32%. Nako ea pula ea LET-ST graphite ke metsotsoana e 139, mme lik'hemik'hale tsa eona tse lekanang le khabone ke boleng ba bohareng har'a merero e meraro ea sebopi sa pele.
- ④ Ha boleng ba LET bo phahame, matla a tšepe a chesang a phahame, mokokotlo oa molomo o mosoeu oa ho lahla tlasa maemo a ts'oanang, le libolo tsa graphite tse ngata; boleng ba LET-ST ke nako ea pula ea graphite. Ha ho etsoa likarolo tse teteaneng le tse kholo, boleng bona ka kakaretso bo hlokahala hore bo be holimo. Ha kholo e ntlafala, ho bolela hore graphite e tsitsipane nakong ea ts'ebetso eohle ea ho tiisa, e leng molemo ho sebelisa matla a ho ikatisa a graphite ho fokotsa shrinkage e sa fellang; karohano ea G1 ke sekhahla sa pula ea austenite ea tšepe e qhibilihisitsoeng. Ha kholo ea G1 e eketseha, tloaelo ea tšepe ea shrinkage porosity e kholo. Ho na le likarolo tse peli tse amang boleng ba G1. Ka lehlakoreng le leng, ke matla a ente le tšepe ea tšepe e qhibilihisitsoeng, ka lehlakoreng le leng, ke khabone e lekanang le tšepe e qhibilihisitsoeng. Ha khabone e lekanang e tšoana, ho ba le phello e ntle ea ente, ho theola boleng ba G1, le tšekamelo ea ho fokotseha e nyane.
- Ka hona, ho bonahala eka seboping sa pele kamora kalafo ea tšepe e qhibilihisitsoeng, khetho C ke eona e ntle ka ho fetisisa, khetho ea B ke ea bobeli, 'me khetho ea A ke e mpe ka ho fetesisa.
Liphetho le puisano ea khetho ea bobeli
C | Si | Mn | P | S | Cu | |
2-1 | 3.70 | 2.36 | 0.18 | 0.007 | - | |
2-2 | 3.66 | 2.39 | 0.19 | 0.005 | - | |
2-3 | 3.46 | 2.65 | 0.18 | 0.005 | - |
Ho latela mekhoa e fapaneng ea ts'ebetso, litšoantšo tse fumanoeng tsa EPIC ke tse latelang:
Mothinya 5: Mothinya oa sebōpi sa bobeli sa pele se entsoeng ka ho qhibilihisoa ka molora oa molora
Mothinya 6: Sephetho sa sebono sa bobeli sa sebōpi A
Mothapo oa 7: Karolo ea sephetho sa lenaneo la bobeli la sebōpi B
Mothapo oa 8: Phello ea lenaneo la bobeli la sebōpi C
- Can E ka bonoa ho tloha mothinya 5 le mothinya 6 hore boleng ba LET bo fokotsoe ho tloha 1149 ho isa 1141 ℃, karohano ea G1 ke 20%, 'me nako ea pula ea LET-ST graphite ke metsotsoana e 146. E kopantsoe le lik'hemik'hale tsa eona, hoa tsebahala hore khabone e lekanang le eona ke sebopi sa bobeli. E phahameng ka ho fetisisa mananeong a mararo. Kamora ho hlahlojoa, boleng bo tlase ba LET ba mothinya oa tšepe oa pele o qhibilihisitsoeng e bile ka lebaka la keketso ea ferrosilicon le graphitizing recarburizer, e hlahisitseng matla a matla a ts'ebetsong a ts'epe ea tšepe e qhibilihisitsoeng.
- Can E ka bonoa ho tloha mothinya 5 le mothinya 7 hore boleng ba LET bo fokotsehile ho tloha 1149 ho isa 1139 ℃, karohano ea G1 ke 24%, 'me nako ea pula ea LET-ST graphite ke metsotsoana e 146. E kopantsoe le lik'hemik'hale tsa eona, hoa tsebahala hore khabone e lekanang le eona ke sebopi sa bobeli. Bohareng ba mananeo a mararo. Lebaka la ho fokotseha ha LET le tšoana le le kaholimo.
- Can E ka bonoa ho tloha mothinya 5 le mothinya 8 hore boleng ba LET bo fokotsehile ho tloha 1149 ho isa 1138 ° C, karohano ea G1 ke 33%, 'me nako ea pula ea LET-ST graphite ke metsotsoana e 144. E kopantsoe le lik'hemik'hale tsa eona, hoa tsebahala hore khabone e lekanang le eona ke sebopi sa bobeli. E tlase ka ho fetisisa likhethong tse tharo.
- Ka kakaretso, moralo oa bobeli oa sebopi sa A o nang le bokhoni bo matla ka ho fetisisa ba nucleation o na le boleng bo phahameng ba LET, tšekamelo e nyane ka ho fetesisa hape ke leano la bobeli la sebopi sa A, mme boleng ba G1 ke bo bonyenyane haholo. E bonts'a hore keketseho ea boleng ba CE e ka fokotsa tloaelo ea ho khutsufala le ho ntlafatsa bokhoni ba nucleation.
Liphetho le puisano ka khetho ea boraro
C | Si | Mn | P | S | Cu | |
3-1 | 3.72 | 2.36 | 0.24 | 0.008 | - | |
3-2 | 3.76 | 2.45 | 0.24 | 0.009 | - | |
3-3 | 3.78 | 2.37 | 0.24 | 0.008 | - |
Mothinya 9: mothinya oa sebopi sa boraro sa pele se entsoeng ka ho qhibilihisoa ka molora oa molora
Mothapo oa 10: Karolo ea sephetho sa lenaneo la boraro la sebōpi A
Mothapo oa 11: Sephetho sa sephetho sa sebopi sa boraro sa B
Mothapo oa 12: Phello ea leano la boraro la sebone sa C.
- Ho tloha mothinya 9 le mothinya 10, ho ka bonoa hore boleng ba LET bo fokotsoe ho tloha ho 1147 ho ea ho 1145 ℃, boleng ba G1 ke 6%, LET-ST graphite Nako ea pula ke metsotsoana e 172.8, e kopantsoe le lik'hemik'hale tsa eona, ea tsebahala hore kh'abone e lekanang le eona ke e tlase ho feta merero e meraro ea sebopi sa boraro.
- Can E ka bonoa ho tloha mothapong oa 9 le mothinya 11 hore boleng ba LET bo theoha ho tloha ho 1147 ho isa ho 1146 ° C, boleng ba G1 ke 10%, 'me nako ea pula ea LET-ST graphite ke metsotsoana e 182.7. E kopantsoe le lik'hemik'hale tsa eona, hoa tsebahala hore khabone e lekanang le eona ke sebopi sa boraro. E phahameng ka ho fetisisa mananeong a mararo.
- Can E ka bonoa ho tloha mothapong oa 9 le mothinya 10 hore boleng ba LET bo fokotsoe ho tloha ho 1147 ho ea ho 1146 ℃, boleng ba G1 ke 9%, 'me nako ea pula ea LET-ST graphite ke metsotsoana e 194.4. E kopantsoe le lik'hemik'hale tsa eona, hoa tsebahala hore khabone e lekanang le eona ke sebopi sa boraro. Bohareng ba mananeo a mararo.
- Boleng ba G1 ka kakaretso ba khetho ea boraro bo batla bo le tlase, ho bontša hore tšepe e qhibilihisitsoeng e qhibilihisitsoeng ke khetho ena e na le tloaelo ea ho nyenyefatsa. Ha re bua ka mokhoa o felletseng, phapang lipakeng tsa tšepe tse tharo tse qhibilihisitsoeng ha e kholo. Ha ho bapisoa, khetho ea boraro ea sebopi A e na le phello e ntle. Qetello ea tlhahlobo ea sampole ke ho sebelisa boleng bo lekanang ba khabone ho fetola sekhahla sa tefiso ka tšepe e qhibilihisitsoeng ea sebopi sa pele le sa bobeli.
Boleng ba LET ba tšepe ea pele e qhibilihisitsoeng ea sebopi sa bobeli bo phahame ho feta sebopi sa pele, mme boleng ba G1 bo nyane ho feta ba sebopi sa pele. Ka ho fetola sekhahla sa tefiso ea sebopi sa bobeli le sa boraro, ho tlosa litšila tse hloekileng tsa manganese ka tšepe ea tšepe, boleng ba LET bo haufi, mme boleng ba G1 bo fokotsehile haholo kamora ho phetoa hape. Ka hona, ho eketsa boleng ba khabone ho ka ntlafatsa bokhoni ba nucleation ea tšepe ea pele e qhibilihisitsoeng mme ea fokotsa.
Tloaelo ea ho fokotseha ha e na phetoho e nyane le mofuta oa lisebelisoa. Ts'ebetso e nepahetseng ea kalafo ea spheroidizing inoculation e fumanoa ka ho bapisa sebōpi sa pele A leano la B le leano la C. Fektheri e ikemetseng ea spheroidizing le inoculant e sebelisa mokhoa o seng o ntse o le teng oa kalafo, mme ts'ebetso ea shrinkage le bokhoni ba nucleation ea tšepe e qhibilihisitsoeng li betere. Mofutsana; Ho ea ka moralo oa bobeli oa sebōpi A, moralo B le moralo C, ha mochini oa spheroidizing moemeli e le 1.2% mme tekanyetso ea inoculant ke 0.5, phello ea kalafo ke eona e ntle ka ho fetisisa, 'me phapang lipakeng tsa keno e kentsoeng pele le ho tlatsoa ha e kholo; feta Ha ho bapisoa merero ea boraro ea sebōpi A, B, le C, ha ho na phapang e totobetseng litlamorao tsa merero e meraro ea kalafo.
Lebaka la phetoho ke boleng ba CE ba tšepe ea pele e qhibilihisitsoeng. Ka bokhutšoanyane, ka boleng bo phahameng ba CE (C3.7-3.9, Si2.1-2.4), a sebelisa Elkem nodulizer inoculant, litekanyetso tsa nodulizer 1.2%, Elkem inoculant 0.5% le phallo ea inoculant e ka fumana sebopeho se phahameng Tšepe e qhibilihisitsoeng e nang le matla a nyutlelie le Tloaelo e tlase ea shrinkage e etsa hore ho be bonolo ho fumana litšepe tsa ductile tse fihlelang litlhokahalo tsa boleng. Qeto ea kopo Morero o tjena: ho qhibiliha boima ba 20t, tefo ea likolobe ea tšepe ea 65%, tšepe ea khale 35%, Elkem nodulizer 1.2%, Elkem inoculant 0.5% + le Flow inoculant, tšepe ea pele e qhibilihisitsoeng C3.7-3.9, Si2.2- 2.5, Mn≤0.3, P≤0.05, S < 0.02, bakeng sa tlhahiso, nka bareng teko bareng khomaretse ho betsa bakeng sa liteko, 'me dissect le boloka' mele lahla. Kamora ho petsoha, bokaholimo ba ts'ebetso bo ile ba hlahlojoa, 'me ho ne ho se na liphoso tsa graphite tse phaphametseng le tse fokotsehileng kamora ho e lokisa, mme lenaneo le atlehile.
Ho phethela
- 1. Likarolo tsa tšepe tse nang le mabota a teteaneng li thata ho li laola tlhahiso ea tšepe ea ductile. Li na le litšobotsi tsa botenya bo boholo ba lebota, ho pholisa butle, ho nang le Mg le likarolo tse ling, le tloaelo e phahameng ea ho fokotseha. Liphoso le litšila nakong ea tlhahiso li bonolo ho etsahala, tse bakang tahlehelo ea moruo. Haholo-holo bakeng sa li-castings tsa sehlopha sa QT400-18AR, litlhoko tsa eona tsa ts'ebetso: ts'ebetso ea ts'ebetso ea ts'ebetso lihlahisoa tsa matla Re≥390; bolelele A≥240; karolelano ea boleng ba tšusumetso KV18≥2, boleng bo tlase ba tšusumetso KV14≥2, le litlhokahalo tse phahameng.
- 2. Ka tlhahlobo e nyane ea liteko tsa sampole, ho tšeloa sengoathoana sa liteko tse nyane ho lekoa likarolo tse fapaneng tsa lik'hemik'hale le mekhoa e fapaneng ea kalafo ea spheroidization inoculation. Sesebelisoa sa Elkem EPIC se lemoha tšekamelo ea tšepe e entsoeng ka ho qhibilihisoa, e khetholla tšebetso e nepahetseng ea lik'hemik'hale le mokhoa o nepahetseng oa kalafo ea nodularization, mme e ka fumana tšepe e qhibilihisitsoeng ka tšekamelo e nyane ka ho fetisisa ea shrinkage.
- 3. Sebelisa lintlha tse fumanoeng tekong e nyane ea ts'ebetso ea tlhahiso ho tlhahiso ea 'nete ho theha moralo o hlakileng le o tsitsitseng oa tlhahiso bakeng sa tlhahiso ea likarolo tse nang le marako a tšepe a ductile. Ka ho hlahloba mochini o lekiloeng oa ho betsa le ho shebella bokaholimo ba sefahleho, ho netefalitsoe hore leano lea sebetsa ebile ho hlahisoa ho entsoe. Boleng bo botle ebile bo fihlela litlhoko tsa boleng.
Ka kopo boloka mohloli le aterese ea sengoloa sena hore se hatisoe hape: Mefuta e Meraro ea Mekhoa ea ho Qhibilihisa le Ho Tšela Bakeng sa Ductile Iron
Minghe Khamphani ea Die Casting li inehetse ho etsa le ho fana ka boleng bo phahameng le likarolo tse phahameng tsa ho lahla likarolo Thining-Wall Die Casting,Hot Chamber Die lahla,Cold Chamber shoa lahla), Tšebeletso e chitja (Die Casting Service,Cnc Machining,Ho Etsa Mofuta, Bokaholimo Phekolo) .Na tloaelo efe kapa efe ea Aluminium die die cast, magnesium kapa Zamak / zinc die casting le litlhoko tse ling tsa castings lia amoheleha ho ikopanya le rona
Tlas'a taolo ea ISO9001 le TS 16949, lits'ebetso tsohle li etsoa ka mechini e makholo ea li-die casting, mechini e 5-axis le lits'ebeletso tse ling, ho tloha ho li-blasters ho isa mechini ea ho hlatsoa ea Ultra Sonic. sehlopha sa baenjiniere ba nang le boiphihlelo, lisebelisoa le bahlahlobi ho etsa moralo oa moreki o phethahala.
Moetsi oa konteraka oa li-cast cast. Bokhoni bo kenyelletsa likarolo tse batang tsa aluminium die die likarolo tsa 0.15 lbs. ho isa ho li-6 lbs., Ho theha phetoho e potlakileng, le machining. Litšebeletso tse kenyellelitsoeng boleng li kenyelletsa ho bentsa, ho thothomela, ho qhekella, ho phatloha ha lithunya, ho penta, ho roala, ho roala, kopano le lisebelisoa. Lisebelisoa tse sebelisitsoeng le tsona li kenyelletsa lits'epe tse kopantsoeng tse kang 360, 380, 383 le 413.
Zinc e shoa ho lahla thuso ea moralo / lits'ebeletso tsa boenjineri tse tšoanang. Moetsi oa moetlo oa li-castings tsa zinc tse nepahetseng. Li-castings tse nyane, li-castings tse phahameng tsa khatello, li-cast cast tsa hlobo, li-castings tse tloaelehileng tsa hlobo, li-unit tsa die le li-cast cast tse ikemetseng le li-cast cast tse tiisitsoeng li ka etsoa. Li-castings li ka etsoa ka bolelele le bophara ho fihlela 24 ho. Ho +/- 0.0005 ho. Mamello.
ISO 9001: Moetsi ea netefalitsoeng oa 2015 oa magnesium ea die die, Bokhoni bo kenyelletsa khatello e phahameng ea khatello ea magnesium die cast to 200 ton room & 3000 kamoreng e batang, moralo oa lithulusi, polishing, molding, machining, powder & liquid paint, QA e felletseng e nang le bokhoni ba CMM , kopano, ho paka le ho tsamaisa.
ITAF16949 e netefalitsoe. Ts'ebeletso e 'ngoe ea ho lahla e kenyeletsa ho lahla lichelete,ho lahla lehlabathe,Matla a khoheli, Lahlehileng bubble lahla,Ho ts'oaroa ha Centrifugal,lephaka lahla,Sa Feleng hlobo lahlaBokhoni bo kenyelletsa EDI, thuso ea boenjiniere, ho etsa mohlala o tiileng le ho sebetsoa ka bobeli.
Lahla Liindasteri Liphuputso tsa likarolo tsa likarolo tsa: Likoloi, libaesekele, lifofane, liletsa tsa 'mino, sesepa sa metsi, lisebelisoa tsa Optical, li-sensor, mehlala, lisebelisoa tsa elektroniki, masaka, lioache, mechini, lienjine, thepa ea ka tlung, mabenyane, mabenyane, telecom, mabone, lisebelisoa tsa bongaka, lisebelisoa tsa litšoantšo, Liroboto, Litšoantšo tse betliloeng, Lisebelisoa tsa molumo, Lisebelisoa tsa lipapali, Lithulusi, Lipapali le tse ling.
Re ka u thusa ho etsa eng ka mor'a moo?
∇ Eya ho Homepage Bakeng sa Shoa lahla China
→Likarolo tsa ho lahla-Fumana seo re se entseng.
→ Malebela a Ralated ka Litšebeletso tsa Die Casting
By Moetsi oa Minghe Die Casting | Categories: Lingoloa tse thusang |lintho tse bonahalang Tags: Aluminium lahla, Ho lahla zinki, Ho lahla Magnesium, Lahleloa thaethaniamo, Ho lahla tšepe, Brass lahla,Ho lahleloa ka Bronze,Ho lahla Video,Histori ea Khamphani,Aluminium Die Casting | Litlhaloso Off